Table 2. Proximate properties of activated carbon derived from the shoot waste of fast-growing teak (FGT)
Thermal treatment (°C) | Heating period (min) | MC (%) | VMC (%) | AC (%) | FCC (%) |
750 | 30 | 6.13d | 17.27d | 5.24d | 77.49b |
60 | 1.12ab | 18.11d | 5.17d | 76.72ab |
90 | 5.07c | 20.38e | 4.77bcd | 74.84a |
750 | 30 | 4.72c | 9.44ab | 4.78bcd | 85.78de |
60 | 1.17ab | 9.84abc | 4.34ab | 85.81de |
90 | 1.28b | 18.32d | 4.52bc | 77.16b |
750 | 30 | 1.45b | 11.63c | 4.88cd | 83.49c |
60 | 0.87a | 11.06bc | 4.69bc | 84.24cd |
90 | 0.84a | 9.16a | 4.03a | 86.80e |
Average | | 2.51 | 13.92 | 4.71 | 81.37 |
SNI 06-3730-1995 | | ≤ 15 | ≤ 25 | ≤ 10 | ≥ 65 |
Groups in a homogenous subset.
MC: moisture content, VMC: volatile matter content, AC: ash content, FCC: fixed carbon content.