Table 4. Weight loss of treated wood exposed to drywood termites

Groups Treatment Weight loss (g)
A0 Nanocellulose (control) 3.18a ± 0.50
A1 Nanocellulose 20% and Metarhizium anisopliae 2.58b ± 0.43
A2 Nanocellulose 40% and M. anisopliae 1.89c ± 0.29
A3 Nanocellulose 60% and M. anisopliae 1.14d ± 0.41
B1 Nanocellulose 20% and Beauveria bassiana 2.39c ± 0.20
B2 Nanocellulose 40% and B. bassiana 2.10d ± 0.13
B3 Nanocellulose 60% and B. bassiana 1.72e ± 0.18
C1 Nanocellulose 20% and Trichoderma harzianum. 3.10h ± 0.43
C2 Nanocellulose 40% and T. harzianum. 2.20i ± 0.33
C3 Nanocellulose 60% and T. harzianum. 1.88j ± 0.20
Different letter ranks indicate a significant difference between treatments.