Table 1.
Recovery of set of pine wood and gmelina wood after the densification process
Wood species
Recovery of Set (%) after immersion in CH
3
COOH-H
2
O
2
at different concentrations
*
15 %
20 %
30 %
Pine
4.72 ± 0.33
3.20 ± 0.07
6.83 ± 1.36
Gmelina
14.04 ± 2.56
12.27 ± 0.67
18.42 ± 2.87
Average and standard deviation of five replicates